Regulation 33, Indian Boiler Regulations, 1950: Plates
Indian Boiler Regulations, 1950 - Regulation 33
Text of regulation 33
Plates
33. Plates—(a) Process.—Tho oox>por shall be nre-refinod or electrolytic, and
hot-rolled from suitable nakes.
(b) Chemical Composition.—The platan shall contain not loss than 99 per oent.
of coppor, and between -3 % and -5 % of arsenic.
(o) Freedom from defects.—Tho plates shall be cloan, smooth and froe from
defects and shall have u workmanlike finish They shall be thoroughly annealed.
(d) Boiling Margin.—No plat a shall bo under the specified thickness at any
part, nor more than 5% over tho calculated weight. The scrap margin, partly
sheared and left attached, shall be no1 lean than 3 inches tit the ends and 1J inches
tiit each Hide.
(e) Tensile Tests.—One tensile tusl shall bo taken from eaoh plato as rolled.
The tensile breaking strength, fi oin Standard Test Piece A, shall not be leas than
14 tons per sq. in. "with an elongation of not loss than 35%.
(f) Hot and Cold Bend teats. -Ono hot (temperature between 1200°T\ and
1400oI\) and ono cold bend test shall bo taken from each plate as rolled.
Tor either hot or cold bend 1estH the test piece •ahall withstand being doubled.
ovei without fraci uro uniil the sides are touching and parallel.