Regulation 83, Indian Boiler Regulations, 1950.: Number of Teste
Indian Boiler Regulations, 1950. - Regulation 83
Text of regulation 83
Number of Teste
83. Number of Teste.— (a) .For type A, one of- tho tests specified in Regulations
69(i»), 59(b) and 5()(c) sball be made from each lot of 250 tubes or fraction thereof
and from eaoh 2,000 ft. or fraction thereof safe end material. For typo C, one of
each of the tests specified in Regulations fi9(a), 59(b), 5!)(o) and 60 shall bo inado from
eaoh lot of 250 tubes or fraction thereof. A reverse bend test specified in Regula-
tion 69(d) shall be uia.de on each 1600 ft. of finished tubing.
(b) ff any test specimen shows dofectivo machining or develops flaws, it may
be discarded and another specimen substituted. j
(o) If the percentage of elongation of any tension tost specimen is less than that
specified in Regulation 60 and any part of the fracture is more than 3/4 in. from the
oontre of tho gauge longth, as indicated by scribe scratohos marked on the specimen
beforo testing, a re-test shall bo allowed.
(d) Eaoh tube shall be subjected to tho hydraulic test speoifled in Regulation
61.
SEC. 3] THE GAZETTE OF INDIA EXTB AOEDINAEY 629
LAPWELDED STEEL BOILER TUBES (FOR EXTERNAL PRESSURE)
64. (a) Material.—The tubes shall bd ,nade from steel which shall show on ana
lysis not more than O'()5 per cent, of ^ulphur or phosphorus. The manufacturer
shall supply a certificate of the analysis AH hen required to do so.
(b) Annealing.—The ends of all tubes shall be carefully annealed .
(c) Freedom from defects.—To comply with Regulation 36(c).
(cl) Tolerances. — The t ibes shall be of the dimensions specified, straight, cylin
drical, of uniform thickness and external diameter throughout, subject to the work
ing margines given in table below :—
Outside diameter of
lube
Under 2 | inch .
2-| inch and over
On diameter
Plus
Inch
1
64
Per cent.
1
Minus
Inch
1
32
Per cent.
1
On thickness
Plus
Per cent.
"1
t 10
Minus
Per cent.
10
on length
Plus
Inch
1/8
Minus
Inch
0
(e) Selection of tubes for test.—To comply with Regulation 37.
65. Tensile test.—(a) To comply with Reg. 44(a).
(b) Flattening test.—To comply with Reg. 44(b), the weld being placed 45°
from the horizontal.
t,c) Expanding test.—r-The selected tubes shall, when cold, withstand being ex-
panded by a drift or a roller expander to the following increases in diameter with-
out showing crack or flaw :—
Thickness of tube 8.W.G.
Up to 10
Above 10 to 6
Above 6 . . . . . . . . . . .
Increase in diameter
per cent.
9-5
7-5
5
66. Additional Tects.—Shrukl a tub<. !-elected for testing purpose, in accordance
with Regulation 37 fail to satisfy the requirements of any one or more of the tests
(specified in Regulations 65(a) (b) (c), if so desired by the manufacturer, the tubes
represented shall be re-annealed and then retested in accordance with these Regula-
tions and if the repeat tests are satisfactory, the tubes shall be accepted provided
that in other respects, they fulfil the conditions of these Regulations, but if the tube
again fails to satisfy the requirements, the tubes which the test pieces represent
shall, be rejected.
67. Hydraulic test.—Every tube shall be tested at the Maker's works by hydraulic
pressure to not less than 1,000 lbs. per sq. in. Any tubes failing to withstand this
test shall be rejected.
^u*U 1-tLj U A Z i j j l l l i Ui . I N l J l A .bjivliJAUxvLU.iNA.Rj. [ l !UlJ- xl
WROUGHT IRON LAPWELDED BOILER TUBES (FOR EXTERNAL
PRESSURE)
68. (a) Material.—The tubes shall b<? made from wrought iron which shall show
on analysis not more than 0*10% manganese and 0"03% sulphur.
(b) Annealing.—The end of all tubes shall bn carefully annealed.
(c) Freedom from defects.—To comply Auth Regulation 36(c).
(d) Tolerance.—Tho tubes shall be of tho dimensions specified subject to working
margins given below. They shall be straight and cylindrical, of unifoim thickness,
concentric and unless otherwise specified, of uniform external diameter through*
out.
The working margin shall be as follows :—
On thickness—plus or minus 10%.
On external dia. for tubes under 2\"—plus 1/64* and minus 1/32".
„ ,, for tubes 2" and larger—plus or minus 1 per cent.
(e) Selection of tufces for test.—To comply with Regulation 37.
69. (a) Tensile Test.—Lengths or strips cut from the selected tubes shall comply
with the following requirements :—
Strips cut from the tubes clear of the welds and
tested in their curved condition
Tested longths taken from finished tubes (ends
of tubes to be plugged for grips)
Ultimate Tensile
Strength in tons/
sq. in.
Not less
than
20
20
Not more
than
24
Elongation per cent,
on 8 in.
10
12*
(b) Flattening Test.—To comply with Regulation 39.
70. Expanding Test.—The selected tubos shall, when cold, withstand being
expanded by a drift or roller expander to the following increases in diameter without
showing crack or flaw:—
Thickness of Tube SWG
Up to 6
Above 6 . . . . . . . .
Increase in Diamoter per cent.
71. Crushing Test.—A ring 2 in. in length cut from one end of each selected
tube shall withstand, without showing crack or flaw, being crushed on end by
hammering or pressure when cold, until the length is reduced to 1-5/8 in.
72. Hydraulic Test.—Every tube shall be tested by internal hydraulic pressure
to not less than 1,000 lbs./sq. in. Any tube failing to withstand this test shall be
rejected.
STEEEL CASTINGS
73. Scope.—Steel castings shall be of the following grades, according to the
purpose for which they are to be used and as may be specified :—
Grade I . . . . . . . 28 to 35 tons per sq. ia.
e»de II 35 to 40 „
, J 1.H..CJ h'ii l i f t L . lnVi-A. . . i . U.
74. (ft) Process of manufacture.—Steel for oastings shall bo made by the Open
Hearth or an Electric Process, acid or basic
(b) Ohemlcal Analysis.—Sto;>l usod for gradoa I and I I castings shall not show
<>u analysis more than 0.06 per cent, of sulphur or phosphorus as determined from
the test samples, and tho manufacturer shall supply an analysis of each oast when
requested.
(c) Heat treatment.—All castings flhall be hoat treated to refine the crystalline
structure throughout tho oasting by heating to a uniform temperature not loss than
the normalising temperature and allowing to cool slowly from the maxirmun tempe-
rature in a praetioally uniform manner: or alternatively normalised by heating in.
a similar manner and allowing to cool in still air.
(d) Freedom from defects.—All castings shall be free from twists, craoks. flaws
and similar defects.
75. Repairs to defective castings.—Casting* shall not bo repaired or weldod with
out the speoino sanction of the Inspecting Officer, If required the castings shall
be suitably re-heattreatod to remove- internal stresses. Should a defect impair the
strength of the castings, ropair by welding or otherwiao shall not bo permitted.
76. Number of tests.—At least one tensile- and one bend test shall be made from
the oaating from each charge, and when more than one casting is made from one
ohargo, at least one tensile and one bend tost stall be made from the castings run
from ono oommon pouring head ; but separate tests shall be made from each oast-
ing or set of castings run from each soparate pouring head.
Test pieces shall riot be cut off until they have been stamped by the Inspecting
Officer after the annealing has been completed.
77. Temile tests. -The ultimate tonsils stress, yield point and elongation for
grades I and I I eastings shall bo not less than shown in table below:—
Tensile Tests on Steel Castings
Omde
I . . . .
II . . . .
Minimum ultimate
Tonsilo Hti'ongth
Tons per aq. in.
28
35
Minimum yiold
point JJI tonnB of
Tonailu strength
por cent.
SO
50
Minimum
Elongation
on test piouo 'C
(figure 5 to Appx, B)
per oent.
20
15
Should a tensile test pieoe break outside the middle half of its gauge length, the
test may at the manufacturer's option be discarded and another test be made of the
same oaating.
78. Bend teats.—Cold bend tests shall bo made upon test pieoos having a rect-
angular seotion of one inch Wide by 3/4 inch thick. The test pieces shall be maohined
and the odgea rounded to a radius of 1/16 inoh. The test pieces shall be bent over th»
thinner section.
632 THE GAZETTE OF TNDTA EXTRAORDINARY [PART II
Bond teats may be made by pj essnni 01 by blows, and tho tost piecesshall without
fraituro withstand being bent lound R forjm r having ft radius of 1 inch through
an angle not Jess thim that given m the following table .—
Braiio orCtiHtuiK 4.ugle of Bund
I . . . . . 00°
II . . . . . l20r
79. Additional teats before rejection. —Should a test pr>er- fir«t wlectod by Hie
luspeotor not fulfil the test roquiremonts, two additional tests of the namo kind from
the sumc easting or group of cawlingfi shall bo made. Should one of the additional
teat pieces fail to fulfil the specified tost requirements, the castings .shall bo rejected.
80. Waiving of tests.—No tests shall be mado from unimportant steel casting
or from Hteol ('listings which aie used lor articles usually made ot cast iron, if the
scantlings are not materially reduced below what would be required if oast iron
were used.
OARRON STEEL TORGINGS
(OTHER THAN 4WAIMLESS DRUMS)
81. (a) Process ot manufacture.—(Jarbon . 1eel for forgings shall be mado by
the Open Hearth or an Electric Process, acid or basic.
(b) Chemical analysis.—Tho steel shall <ontain not more than 0-05 par eeul. ot
sulphur or of phosphorus.
(c) Fresdom from detects. -Til** forpingH shall be froo from defects ot any kind
and shall bo finished to the prescribed dimensions. Defects m forgings, shall not
be repaired without the previous .sanction of tho Inspecting Officer,
(d) Heat treatment.—Kadi forging shall bo efficiently h'vit-tioated unless
during the last stage of mauiifactute it has been finished at such n temperature as to
ensure that tho mateiial ot tho foigmg •will have satisfactory meehunical proper-
ties.
82. Selection of teat pieces.—Hiiftu iont material shrill be left on oa< h forging for
test pieces. In the case of a number of small forgings, not less (linn two per cent,
of (he total or not lesR than 2 forgings from each cast.
83. (a) Tensile tests. —The ultimate tenmlo wtroHs and elongation shall bo between
the limits of 26 and 32 Tons per sq. in and 28% and 22% respectively determined on.
Butmh Standard Test Piece 0, or subsidiary Standard Round Test Piece (See
Appendix B.)
In no case shall the sum of the ultimate tensile Htrows and corresponding < longa-
tion be loss than 54.
(b) Should a tonailr) t'»st pieoe break outside tho middl i half of the test
gauge length the test may, at the maufacturor's option, bo discarded and anothei
test be made of tho name forging.
Previous and next
Questions people ask
Is regulation 83 of Indian Boiler Regulations, 1950. still in force?
No repeal of Indian Boiler Regulations, 1950. is recorded.