LawGrids logoLAWGRIDS.ORG

Appendix D, Indian Boiler Regulations, 1950.: APPENDIX D

Indian Boiler Regulations, 1950. - Appendix D

Text of appendix D

APPENDIX D

APPENDIX D Proof Test for Creep Quality of Carbon Steel plate of Boiler Plate Qaality SPECIFICATION NATTTBE OP TBST 1. The tost shall consist of a tensile oreop tost carried out over a period of at least 48 hours at a temperature of 450°C. and with a stress of 8 tons per fiq. in. Under these conditions the slope of the ohord to the creep curve between the 24th and 48th hour shall not exceed 60 X 10-* strain por hour. CONDITION OF MATERIAL 2. The test shall bo made on the material in the normalised condition. The normalising temperature shall be bewteen 875°C.—926°C, and the plate sample shall be maintained ai the normalising temperature for one hour per inch of thickness and cooled freely in stdl air. TBMPHBATUBH or TSET !3. (iv) Temperature, measurement.-—The temperature of the specimen shall be measured by thermocouples suitable for the temperaturo specified. Two thermo- couples situated one at each end of the gauge length shall be used in the case of test pioces having gauge lengths up to 2 in., and for longer gauge lengths an additional thermocouple situated nt the middle of the gauge length shall be used. Thermocouples nhall make good thermal contaot •with the test piece and be protected from the direct heat of the furnace by being covered with asbestos tape or equivalent insulation. The cold junction shall be maintained at a known temperature which shall bo registered by a mercury thermometer. Alternatively, a suitable means shall be provided for correcting automatically errors in reading duo to changes in tempera- ture of the cold junction. (b) Temperature control.—The two (or throe) thermocouple specified in clause S (a) shall agree with one another within 3 T . and the average of these readings shall be taken as the tost temperature which shall not vary from 450°O. by more than± 2°C. throughout the tost. Either a continuous record or sufficient readings of the temperaturo shall bo made to indicate that the temperature conditions have been satisfactory. (o) Heating feriod before loading.—-Tho specimen shall be maintained at the specified temporatuio for at least an hour prior to the application of the load. STRESS 4. The load required to produce the specified stress shall be gradually applied without shook during a period not excelling five minutes and the stress shall be aocur te to : j I 2 | per cent. SENSITIVITY OF STBAIN-MEASUEINO EqurrMEnT 5. The sensitivity of the extensometci must be such that strains can be mea- sured to the nearest 0-00002. READINGS 6. A sufficient number of strain readings shall be taken clearly to define the creep curve up to 48 hours, and the uhrtrd slope shall be measured from a chord drawn between points on the ourve at the 24th and 48th hours. 8S0 THE GAZETTE OF TNDlA EXTRAORD1NAEY [PAUI TL REPEAT TEST 7. If the material fitilH t<i pass the teat, but (ho choid slope dooti not oxeecd OOx 10-" strain, per hour, a re-test may be made at the request of tJie niunufactuicr and shall be accepted if -satisfactory, or at the Jnapector'n discietion a puss test at a stress f> por cent less than that specified may be accepted,

Previous and next

All provisions of Indian Boiler Regulations, 1950.

Questions people ask

Is appendix D of Indian Boiler Regulations, 1950. still in force?

No repeal of Indian Boiler Regulations, 1950. is recorded.